Process Information Polymer
PA 2200 on HELIOR
Product Description
The process data sheet shows the property values for the solution combination of EOS Helior and PA 2200.
| MECHANICAL PROPERTIES | DRY / CONDITIONED | UNIT | TEST STANDARD | DRY / CONDITIONED | UNIT | TEST STANDARD |
|---|---|---|---|---|---|---|
|
Tensile Modulus X Orientation Y Orientation Z Orientation |
1950 / 1550 1950 / 1550 1900 / 1500 |
MPa MPa MPa |
ISO 527-1/-2 |
1950 / 1600 1950 / 1600 1950 / 1600 |
MPa MPa MPa |
ASTM D 638 |
|
Tensile Strength X Orientation Y Orientation Z Orientation |
52 / 47 52 / 47 51 / 46 |
MPa MPa MPa |
ISO 527-1/-2 |
50 / 45 50 / 45 49 / 44 |
MPa MPa MPa |
ASTM D 638 |
|
Strain/Elongation at Break* X Orientation Y Orientation Z Orientation |
10 / 17 10 / 17 10 / 16 |
% % % |
ISO 527-1/-2 |
17 / 28 16 / 22 16 / 22 |
% % % |
ASTM D 638 |
|
Charpy Impact Strength (+23°C) X Orientation Y Orientation Z Orientation |
30 / 36 29 / 33 26 / 29 |
kJ/m² kJ/m² kJ/m² |
ISO 179/1eU | - | - | - |
|
Charpy Impact Strength (-30°C) X Orientation Y Orientation Z Orientation |
28 / - 31 / - 25 / - |
kJ/m² kJ/m² kJ/m² |
ISO 179/1eU | - | - | - |
|
Charpy Notched Impact Strength (-30°C) X Orientation Y Orientation Z Orientation |
3.1 / - 2.8 / - 2.4 / - |
kJ/m² kJ/m² kJ/m² |
ISO 179/1eA | - | - | - |
|
Izod Impact Strength (+23°C) Z Orientation |
22 / - |
kJ/m² |
ISO 180/1U | - | - | - |
|
Izod Notched Impact Strength (+23°C) X Orientation Y Orientation Z Orientation |
- / - - / - 4 / - |
kJ/m² kJ/m² kJ/m² |
ISO 180/1A |
40 / 42 41 / 45 41 / 44 |
J/m J/m J/m |
ASTM D 256 |
|
Shore D Hardness X Orientation |
77 / - |
- |
ISO 7619-1 | - | - | - |
*
Depending on the material’s fracture behavior, the reported strain value corresponds either to the strain at break (εb) for brittle materials or to the nominal strain at break (εtB) for ductile materials.
| THERMAL PROPERTIES | DRY / CONDITIONED | UNIT | TEST STANDARD | DRY / CONDITIONED | UNIT | TEST STANDARD |
|---|---|---|---|---|---|---|
| Melting Temperature | 176 | °C | ISO 11357-1/-3 | - | - | - |
| Temperature of Deflection under Load 1.80 MPa | - | - | ISO 75-1/-2 | - | - | - |
| Temperature of Deflection under Load 0.45 MPa | - | - | ISO 75-1/-2 | - | - | - |
| Vicat Softening Temperature | - | - | ISO 306/B50 | - | - | - |
| ELECTRICAL PROPERTIES | DRY / CONDITIONED | UNIT | TEST STANDARD | DRY / CONDITIONED | UNIT | TEST STANDARD |
|---|---|---|---|---|---|---|
|
Comparative Tracking Index CTI X Orientation Y Orientation Z Orientation |
≥600 / - ≥600 / - ≥600 / - |
|
IEC 60112 | - | - | - |
|
Surface Resistivity X Orientation Y Orientation Z Orientation |
2E16 / - 2E16 / - 2E16 / - |
Ohm Ohm Ohm |
DIN EN 62631-3-2 | - | - | - |
|
Volume Resistivity X Orientation Y Orientation Z Orientation |
6E14 / - 6E14 / - 8E14 / - |
Ohm•m Ohm•m Ohm•m |
DIN EN 62631-3-1 | - | - | - |
| FIRE PERFORMANCE ELECTRICAL & ELECTRONICS |
RESULT | CONDITION / UNIT | TEST STANDARD |
|---|---|---|---|
| UL 94 Flammability Rating | HB, Test passed | class | UL 94 |
| Thickness Tested | 0.5 | mm | - |
| UL 94 Flammability Rating | HB, Test passed | class | UL 94 |
| Thickness Tested | 1.6 | mm | - |
| UL 94 Flammability Rating | HB, Test passed | class | UL 94 |
| Thickness Tested | 3.2 | mm | - |
| OTHER PROPERTIES | VALUE | UNIT | TEST STANDARD | VALUE | UNIT | TEST STANDARD |
|---|---|---|---|---|---|---|
| Density | 0.98 | g/cm³ | DIN EN ISO 1183-1 | - | - | - |
| Color of parts | weiß | - | - | - | - | - |
| Yellowness Index (YI) | -2.8 | - | ASTM E 313 | - | - | - |
| Powder Color | white | - | - | - | - | - |